Electrodes ENiCrFe-3 maka Nickel

Nkọwa Dị Mkpirikpi:

Electrode na-etinye 65Ni-20Cr-2Nb-1.5Mo ígwè weld.


Nkọwa Ngwaahịa

Akara Ngwaahịa

Koodu EN ISO: 14172: ENi6082

Electrode na-etinye ígwè weld 65Ni-20Cr-2Nb-1.5Mo. Ọ dị mma maka igwe weld dị iche iche nke nwere ihe ndị dị elu. Ọ dabara nke ọma maka igwe weld dị iche iche nke nwere ihe ndị yiri ya, maka igwe e ji Nickel-Chromium-Iron mee mgbe ihe dị n'ime ya dị elu anaghị emerụ ahụ, maka igwe e ji Nickel Chromium-Iron mee na ngwakọta ígwè dị iche iche. Ọ dabara adaba maka mkpuchi efere forge. A na-atụ aro ya nke ọma maka ịgbado ọkụ 9% Ni Steels maka ọrụ cryogenic. A na-ejikwa ya maka ịgbado ọkụ nke alloys Nickel-Chromium ejiri mee ihe maka ojiji okpomọkụ dị elu dị ka ihe ndị na-ekpo ọkụ ọkụ na tubes reformer.

Ihe mejupụtara kemịkalụ nkịtị nke ígwè niile e ji welded mee

Ihe C Mn Si Cr Ni Fe Nb Cu Ti S P
Pasentị ≤0.10 5.0-9.5 ≤1.0 13.0-17.0 ≥59.0 ≤10.0 1.0-2.5 ≤0.50 ≤1.0 ≤0.015 ≤0.030

ÀGWÀ MGBE A NA-AHỤ N'IME ÍGWÈ NKE ÍGWÈ NIILE

UTS YS Ogologo Ike Mmetụta CVN (J) Mgbasawanye Mpụta Ike Na-agbagharị agbagharị na
(MPa) (MPa) (L= 5d)% na Mbelata 196°C na mwepu 196°C (mm) 600°C ruo awa 1000.
620 500 30 75 0.85 160 MPa

DATA UGBU A NA NKWAKỌTA: DC (+)

Nha (mm)

Dia x Ogologo

5 × 350

4×350

3.15 × 350

2.5 × 350

Oke Ugbu a (Amps)

150-180

120-150

80-110

Afọ 60-70

Ibu/Katọn (kg)

2.5

2.5

2.5

2.5

Ịkpachara Anya

1. Hụ na elektrọd ndị ahụ kpọrọ nkụ. Kpoo elektrọd ndị ahụ ọzọ na 300-325°C ruo otu awa.

2. Debe obere arc, eriri stringer ma belata ihe na-etinye okpomọkụ.

3. Hapụ ihe e ji agwakọta ya ka ọ jụọ oyi ruo n'okpuru 50 Celsius tupu ọ tinye ya, oyi akwa ọzọ.